Typical Elevated Temperature Tensile Properties Alloy 321 (0.036 inch thick / 0.9 mm thick) | |||||
Test Temperature | Yield Strength .2% Offset psi (MPa) | Ultimate Tensile Strength psi (MPa) | % Elongation in 2 in. | ||
°F | °C | ||||
68 | 20 | 31,400 (215) | 85,000 (590) | 55.0 | |
400 | 204 | 23,500 (160) | 66,600 (455) | 38.0 | |
800 | 427 | 19,380 (130) | 66,300 (455) | 32.0 | |
1000 | 538 | 19,010 (130) | 64,400 (440) | 32.0 | |
1200 | 649 | 19,000 (130) | 55,800 (380) | 28.0 | |
1350 | 732 | 18,890 (130) | 41,500 (285) | 26.0 | |
1500 | 816 | 17,200 (115) | 26,000 (180) | 45.0 |